2205 Duplex Stainless Steel: Composition, Properties & Uses

2205 duplex (UNS S32205 / S31803) is a two-phase stainless steel with a roughly 50/50 austenite-ferrite structure. With about 22% chromium, 3% molybdenum and added nitrogen, it combines roughly twice the yield strength of 304/316 with excellent resistance to pitting, crevice corrosion and chloride stress-corrosion cracking. Yuhang Metal supplies 2205 duplex pipes, tubes, sheets and plates to ASTM and EN standards with EN 10204 3.1 certification.

Quick answer: 2205 duplex is about twice as strong as 304 or 316 (minimum yield strength 450 MPa against 205 MPa) and resists chloride pitting and stress-corrosion cracking much better than 316L. Use it for chloride-bearing process piping, heat exchangers, desalination equipment and marine structures.

Chemical composition (S32205, max % unless range)

CMnSiPSCrNiMoN
22050.0302.001.000.0300.02022.0–23.04.5–6.53.0–3.50.14–0.20

Mechanical properties (annealed, ASTM A240 minimums)

Tensile strengthYield strength (0.2%)Elongation
2205 (S32205)≥ 655 MPa (95 ksi)≥ 450 MPa (65 ksi)≥ 25%

Equivalent designations

UNSENJIS
2205S32205 / S318031.4462 (X2CrNiMoN22-5-3)SUS329J3L

Typical applications

Heat exchangers and pressure piping with chloride-bearing media, desalination and water treatment, chemical tankers and storage tanks, structural members in marine environments, and pulp & paper equipment.

Why specify duplex

The high yield strength often allows thinner walls than an austenitic design, reducing weight and material cost, while the pitting resistance (PREN around 35) and resistance to stress-corrosion cracking outperform 316L in chloride service. Welding requires qualified procedures to keep the phase balance; our OEM team fabricates to your drawing and WPS requirements.

Pitting resistance (PREN)

PREN (pitting resistance equivalent number) = %Cr + 3.3 × %Mo + 16 × %N. It ranks resistance to chloride pitting: the higher the number, the better. 2205 (S32205) has a calculated PREN of about 34.1–37.8, compared with about 22.6–29.5 for 316/316L. Values are calculated from the ASTM A240 composition limits. PREN is a ranking tool, not a guarantee of performance in a particular environment.

How to check you received 2205 duplex

A handheld XRF analyser confirms chromium (22–23%), nickel (4.5–6.5%) and molybdenum (3.0–3.5%). XRF cannot measure nitrogen, so check it on the mill certificate. Duplex material can also be checked for ferrite content with a ferrite meter and, where the order specifies it, tested to ASTM A923 for detrimental intermetallic phases. See our pre-shipment inspection guide.

Frequently asked questions

Is 2205 duplex stainless steel magnetic?

Yes. About half of its structure is ferrite, which is magnetic. This is normal for duplex and not a sign of the wrong grade.

What is the difference between S31803 and S32205?

Both are 2205 duplex. S32205 has higher minimum chromium, molybdenum and nitrogen (22.0% Cr, 3.0% Mo, 0.14% N) than S31803 (21.0% Cr, 2.5% Mo, 0.08% N). Material that meets S32205 also meets S31803, so it is often dual-certified.

What is the maximum service temperature for 2205 duplex?

ASME pressure vessel codes restrict duplex stainless steels to service below about 315 °C (600 °F), because longer exposure at higher temperatures makes them brittle. Some other codes set lower limits.

2205 duplex products from Yuhang Metal

Pipes & tubes · Sheets & plates · Tube coils · Custom & OEM fabrication

Request a quotation

Send us the product form, dimensions, quantity and standard (ASTM, EN or JIS). Every delivery includes an EN 10204 3.1 mill test certificate. Request a quote.